OSP

OSP (Organic Solderability Preservative) protects bare copper pads with an ultra-thin 0.2–0.5 µm organic film. During reflow the film is consumed by flux, so solder wets clean copper directly — a flat, RoHS-compliant finish at the lowest cost of any lead-free option.

0.2–0.5 µm

Film thickness

3–12 mo

Shelf life, vacuum-sealed

1–3×

Reflow cycles

100%

RoHS & lead-free

What is OSP?

OSP is a water-based chemical finish applied to bare copper. It deposits an ultra-thin organic film (azole chemistry) that bonds with copper ions and blocks oxidation during manufacturing and storage — then dissolves in the reflow flux to expose fresh copper for a strong solder joint.

Non-metallic & transparent

No plating layers, no thickness buildup — pads stay flat and copper-colored.

Consumed by flux

The film vanishes during soldering, leaving no residue on the finished joint.

Direct copper bond

Solder wets clean copper for strong intermetallic joints — no black-pad risk.

Lead-free & eco-friendly

Water-based chemistry, fully RoHS compliant and safe for disposal.

How it protects — and how it lets go

01
Bare copper
Clean copper pads, ready for protection.

02
OSP film
Thin organic layer blocks oxygen & humidity.

03
Flux dissolves
During reflow the film breaks down.

04
Solder wets copper
Molten solder bonds directly to fresh copper.

Key specs at a glance

Values reflect typical production chemistry and packaging. Your specific OSP grade is confirmed at quotation.

ParameterOSP
Film thickness0.2–0.5 µm (200–500 nm)Self-limiting azole film on copper pads only
Surface flatnessExcellentConformal coating — no solder domes, ideal for fine-pitch and BGA
Shelf life3–12 monthsVacuum-sealed with desiccant; depends on chemistry grade & storage
RoHS / lead-freeYesWater-based, non-metallic chemistry
Thermal cycles1–3 reflows typicalUp to 4 passes (2 reflow + 2 wave) with high-grade chemistry
Relative costLowMost economical flat lead-free finish; no precious metals
SolderabilityExcellent when freshFlux dissolves the film; solder wets clean copper

Testing on every lot

XRF thickness measurement on production lots

Cross-section analysis of the layer build-up

Solderability and adhesion testing

Salt spray, porosity and wire-bond pull per spec

Black-pad prevention

Mid-phosphorus nickel bath (7–9% P)

Controlled immersion time and bath turnover (MTO)

Statistical process control with out-of-range alarms

XRF thickness measurement on production lots

How OSP is applied - Process in 6 steps

OSP runs on an automated conveyor line: clean, micro-etch, coat, rinse, dry. The whole cycle takes minutes, which is why it scales so well to high-volume production.

STEP 01

Degrease & clean

Alkaline degreaser removes oils, oxides and fingerprints for uniform wet-out.

STEP 02

Micro-etch

Removes ~1.0–1.5 µm of copper, roughening the surface for strong film adhesion.

  1.0–1.5 µm removal  

STEP 03

Acid rinse & activate

Neutralizes etch residues and prepares the copper for organometallic bonding.

STEP 04

OSP coating

Immersion in the OSP bath deposits the protective organic film.

  25–40 °C · 30–120 s  

STEP 05

DI water rinse

Deionized rinse removes unreacted chemistry and ionic contamination.

STEP 06

Hot-air dry

Clean heated air sets the film to a smooth, transparent finish.

  60–80 °C   

1.0–1.5 µm
Micro-etch copper removal
25–40 °C · 30–120 s
OSP bath temperature & dwell
0.2–0.5 µm
Final film thickness target

The honest engineering view - Pros & cons

Why teams choose OSP

Lowest-cost flat lead-free finish available

Excellent flatness for fine-pitch, QFN and BGA

RoHS-compliant, lead-free, water-based chemistry

Strong solder joints — solder wets clean copper directly

No black-pad risk (no nickel layer involved)

Fast process, stable yield, ideal for high volume

Where OSP needs care

Shorter shelf life than metallic finishes (3–12 months)

Sensitive to moisture, handling and contamination

Limited to 1–3 reflow cycles in practice

Transparent film is harder to inspect visually

Not for edge connectors, gold fingers or harsh environments

Pick the finish that fits your board

A quick side-by-side of the three most common finishes. Cost and flatness are relative — exact figures depend on board size, quantity and stack-up.

actorOSPENIGHASL (lead-free)
Relative costLowNo precious metalsHighNickel + goldLow
Surface flatnessExcellentExcellentPoorUneven solder domes
Shelf life3–12 monthsChemistry & packaging dependent12+ months~12 months
BGA / fine-pitchGood–ExcellentFlat, but reflow-limitedExcellentIndustry benchmarkNot recommended
Multiple reflowsLimited (1–3)ExcellentHigh
RoHS / lead-freeYesYesYes
Best forHigh-volume consumer SMTHigh-reliability, long storageThrough-hole, low-density

Choose OSP when

High-volume production, per-unit cost matters

Fine-pitch SMT, QFN or BGA with a short storage window

Boards assemble within weeks of fabrication

RoHS / lead-free compliance is mandatory

Where OSP belongs — and where it does not

Two quick checklists so you can decide in seconds whether OSP fits your product.

Good fit for OSP

Consumer electronics & wearables

IoT and smart-home modules

LED lighting boards

Automotive electronics (non-harsh zones)

High-density SMT, fine-pitch QFN / BGA

High-volume assemblies with fast turnaround

Choose another finish

Edge connectors or gold fingers (no wear resistance)

Outdoor or high-humidity environments

Long inventory storage before assembly

Frequent rework or multi-pass assembly

Contact surfaces requiring repeated use

Four rules that keep OSP solderable

OSP is a discipline finish. Follow these four rules and solderability stays intact through assembly.

Store cool & dry

20–25 °C, relative humidity below 60%, away from acids and heat.

Keep vacuum-sealed

Boards ship in moisture-barrier bags with desiccant and humidity indicators.

Assemble fast after opening

Complete SMT within 24–48 hours once the vacuum bag is opened.

Handle with gloves

ESD nitrile gloves only — skin oils and salts dissolve the film.